X-ray testing of welds resolves volume defects well and planar defects badly. Gas pores, slag inclusions and shrinkage cavities change the thickness of material along the beam, so they show as density differences; lack of fusion and a crack lying unfavourably to the beam may change almost nothing in the image. That single limitation decides more specifications than tube power does. This page applies to conventional steel, aluminium and cast components examined by radiography; it does not set your acceptance level or make a compliance judgement for you. It covers defect detectability, how thickness sets energy, what the standards actually specify, image-quality indicators, and the cases where another NDT method is required.
Radiography responds to a change in attenuation along the ray path. A defect with volume in the beam direction removes or adds material and produces contrast; a tight planar discontinuity parallel to the beam may remove almost none, so a crack can be present in a weld that looks clean on the film or detector.
Defect type, radiographic detectability, and the condition attached to it
Defect | Detectability by radiography | Condition |
Gas porosity, blowholes | Usually clear | Volume is large enough relative to section thickness and image quality |
Slag or dense inclusions | Usually clear | Inclusion density differs from the surrounding metal |
Shrinkage cavities in castings | Usually clear | Cavity lies within the penetrated thickness range |
Lack of side-wall fusion | Unreliable | Depends on orientation to the beam and on joint geometry |
Tight cracks, cold shuts | Often missed | Planar and unfavourably oriented; may need a second angle or another method |
The practical consequence is that exposure geometry is part of the inspection, not a setup detail. Where a planar defect is the concern, additional beam angles or a different method have to be specified in the procedure. A single radiograph taken at the most convenient angle cannot be used to conclude that a weld is free of lack of fusion, and no amount of detector resolution changes that.
Energy is set by the densest and thickest section in the beam. Steel needs more than aluminium at the same thickness, and a stepped or cored casting needs more than a uniform plate. Tube voltage is therefore chosen for penetration first; exposure time and filtration are then adjusted to bring the detector into a usable range without flattening the contrast of small defects.
Raising voltage has a cost. As the beam becomes more penetrating, the difference in attenuation between a small pore and the surrounding metal shrinks, so the defect that was visible at a lower energy can disappear. The working rule is to use the lowest energy that still penetrates the thickest section with an acceptable image quality indicator reading, not the highest voltage the tube can produce. The published weld X-ray inspection machine pages list maximum voltage as a capability bound; the setting for a given part still has to be established on that part.
Geometry matters as much as energy. A flange, a boss or a change in section inside one field of view creates a wide range of path lengths, and a single exposure may not cover both the thin and thick regions. Where that spread is large, plan for multiple exposures or for masking rather than expecting one image to hold the whole dynamic range.
Standards specify the method, the image quality and the recording of results; they do not tell you that a particular weld is acceptable. That judgement comes from the acceptance level in the contract, the applicable code and your own quality system, applied by the responsible personnel.
For welds, the ISO 17636 series describes radiographic testing of fusion-welded joints and the image-quality requirements that go with it. For castings, ASTM E1032 covers radiographic examination and reference radiographs such as ASTM E505 are used to compare indications. ASTM E94 is widely cited as a guide to radiographic practice. Each of these documents defines scope, technique and image quality rather than a universal pass line. Use the edition named in your own procedure — editions and the acceptance levels referenced from them change, and a brochure that says "complies with ISO 17636" is not a statement about your part.
A site page on weld X-ray machine selection covers equipment choice; the standards question is separate and should be settled first. If the procedure calls for a technique class, an image-quality indicator value or a specified source-to-film distance, the equipment has to support those conditions, not the other way round.
An image quality indicator (IQI, sometimes called a penetrameter) verifies the quality of the image, not the quality of the weld. It is a small calibrated object with known wires or holes placed on the part; if the required wire or hole is visible in the radiograph, the combination of energy, geometry, detector and exposure reached the sensitivity the procedure demands.
That distinction is easy to lose on a production floor. A readable IQI tells you the radiograph could show a discontinuity of a certain size under those conditions. It does not say the part is sound, and it does not compensate for a planar defect oriented away from the beam. Place the indicator on the source side at the thickest relevant section, and record which element was visible together with the exposure conditions, so a later image can be compared against the same baseline.
The technique is described in the site's material on radiography of castings. Where the section thickness varies a lot across one image, more than one indicator position may be needed to demonstrate sensitivity across the whole field.
Match the machine to the thickest section, the largest part and the geometry the procedure requires — in that order. A compact precision casting system suits small, thin-walled parts where fine detail matters; a general industrial system suits mixed weldments and larger components where penetration and room to position the part dominate.
The published pages give three distinct configurations to compare: X-ray casting inspection equipment for precision cast parts, the XCT8500 universal industrial system for mixed work, and the XPT8200 multi-purpose high-resolution system where both radiography and 3D capability are needed. On each page, check maximum penetration, available tube voltage range, detector area, and the working envelope for the part and the image quality indicator together. A machine that fits the part but leaves no room for the indicator or the required source-to-detector distance will not produce a valid technique.
Do not choose on detector resolution alone. For a thick steel section, penetration and exposure geometry decide what can be seen long before pixel pitch does.
Use another NDT method when the expected defect is planar, when access to both sides of the part is impossible, or when the geometry prevents a usable beam path. Ultrasonic testing is better suited to tight cracks and lack of fusion, particularly in thicker sections; dye penetrant or magnetic particle inspection handles surface-breaking discontinuities more directly. Radiography also brings shielding, exclusion zones and regulatory obligations that a surface method does not.
General references on X-ray NDT equipment describe the method's scope, but the decision here is about the failure mode: if the concern is a crack that can lie parallel to the beam, an X-ray image is the wrong evidence. Saying so early avoids buying a capable machine for a question it cannot answer.
A sensible specification names both the method and the exclusion. Write down which discontinuities radiography is expected to find, which are covered by a second method, and what triggers a re-examination at a different angle. That record is more useful than any single equipment parameter.
That depends on the product code, the contract and the edition cited in your quality system. The ISO 17636 series and the ASTM documents cover method and image quality, not a universal acceptance level. Confirm the applicable edition and acceptance criteria with the person responsible for the welding procedure before specifying equipment.
Often not. Castings vary in section thickness and may need multiple exposures or reference radiographs; welds are usually examined along a defined seam with a specified beam angle and technique class. The energy, geometry and acceptance references differ even when the same cabinet is used.
It can produce an image of a thin, low-density sample, but it is not a substitute for a qualified radiographic technique. Tube voltage, penetration, image-quality indicators, shielding and the procedure's recording requirements are all different. Use equipment configured for the material and section you need to assess.
ISO 17636 series (radiographic testing of welded joints), ASTM E94 (radiographic examination guide), ASTM E1032 (radiographic examination of castings), ASTM E505 (reference radiographs for aluminium and magnesium castings). Edition and acceptance level are determined by the reader's own procedure; no compliance claim is made here.
Seamark ZM published product pages: XD160 precision casting inspection equipment, XCT8500 universal industrial X-ray inspection system, XPT8200 multi-purpose 3D system, offline X-ray inspection machines.
Internal guides on this site: weld X-ray inspection standards, choosing a weld X-ray inspection machine, casting inspection techniques, and X-ray inspection equipment principles.
EN
es
ko
de
it
pt
th
ar
pl
vi
tr
ru